Open access

Biomass Feedstock Pre-Processing – Part 1: Pre-Treatment

Written By

Lope Tabil, Phani Adapa and Mahdi Kashaninejad

Submitted: 18 October 2010 Published: 01 August 2011

DOI: 10.5772/17086

From the Edited Volume

Biofuel's Engineering Process Technology

Edited by Marco Aurélio dos Santos Bernardes

Chapter metrics overview

9,381 Chapter Downloads

View Full Metrics

1. Introduction

1.1. Sources of biomass

The two main sources of biomass for energy generation are purpose-grown energy crops and waste materials (Larkin et al., 2004). Energy crops, such as Miscanthus and short rotation woody crops (coppice), are cultivated mainly for energy purposes and are associated with the food vs. fuels debate, which is concerned with whether land should be used for fuel rather than food production. The use of residues from agriculture, such as barley, canola, oat and wheat straw, for energy generation circumvents the food vs. fuel dilemma and adds value to existing crops (Chico-Santamarta et al., 2009). In fact, these residues represent an abundant, inexpensive and readily available source of renewable lignocellulosic biomass (Liu et al., 2005).

1.2. Current issues related to biomass utilization

The main problem with agricultural straw is its relatively low density in its original or baled forms. The bulk density of loose and standard baled straw is approximately 40 kg/m3 and 100 kg/m3, respectively, compared with the bulk density of unprocessed wood residue, which is approximately 250 kg/m3 (Demirbaş, 2001; Tripathi et al., 1988). The relative low density of straw makes it more expensive to transport compared to wood and coal because a lower mass of straw can be transported per unit volume. Additionally, a larger storage area/volume is required for baled straw compared to wood chip. Densification into pellets increases the bulk density of biomass (McMullen et al., 2005; Obernberger and Thek,2004) and as a result, the net calorific content per unit volume is increased (Bhattacharya et al., 1989) and the storage, transport and handling of the material is easier and cheaper (Balatinecz, 1983; Bhattacharya et al., 1989; Kaliyan and Morey, 2006).

The quality of fuel pellet is usually assessed based on its density and durability. High bulk density increases storage and transport capacity of pellets (Adapa et al., 2007; Mani et al., 2003). Since feeding of boilers and gasifiers generally is volume-dependent, variations in bulk density should be avoided (Larsson et al., 2008). A bulk density of 650 kg/m3 is stated as design value for wood pellet producers (Obernberger and Thek 2004). Low durability of pellets results in problems like disturbance within pellet feeding systems, dust emissions, and increased risk of fire and explosions during pellet handling and storage (Temmerman et al. 2006).

Densification of straw and determining the optimal parameters involved is an art in itself. The entire process involves securing of baled straw from agricultural fields, size reduction (chopping and grinding), application of pre-treatment (chemical, physico-chemical, and biological), determining the physical and frictional properties of straw grinds, lignocellulosic characterization of straw, lab-scale and pilot-scale densification of grinds into pellets to determine the effect of various independent parameters on quality (density and durability), and energy analysis/ balance (Fig. 1). This chapter will only address the effect and need of lignocellulose characterization, pre-treatment and size reduction, and physical properties on densification of agricultural straw.

Figure 1.

Processing steps involved in converting straw from field to pelletized product.

Advertisement

2. Lignocellulosic biomass characterization

2.1. Structure of lignocellulosic material

Lignocellulosic material refers to plant biomass that is composed of cellulose, hemicellulose, and lignin (Fig. 2) (Lin and Tanaka, 2006). The major combustible component of non-food energy crops is cellulose, followed by lignin.

Cellulose: Cellulose is an organic polysaccharide consisting of a linear chain of several hundreds to over nine thousand β(1→4) linked D-glucose (C6H10O5)n units (Crawford, 1981; Updegraff, 1969). Cellulose, a fibrous, tough, water-insoluble substance, is found in the cell walls of plants, particularly in the stalks, stems, trunks and all the woody portions of the plant body (Nelson and Cox, 2005). Cellulose comprises 40-60% of the dry weight of plant material (the cellulose content of cotton is 90% and that of wood is 50%) (Encyclopædia Britannica, 2008; USDE, 2006).

Zandersons et al. (2004) and Shaw (2008) reported that binding of wood material during hot pressing / densification is mainly dependent on the transition of cellulose into the amorphous state. According to Hon (1989), due to the semi-crystalline structure, hydrogen bonded cellulose cannot be dissolved easily in conventional solvents, and it cannot be melted before it burns; hence, cellulose itself is not a suitable adhesive. This can be overcome by breaking the hydrogen bonds, thus making the cellulose molecule more flexible (Hon 1989). Cellulose requires a temperature of 320°C and pressure of 25 MPa to become amorphous in water (Deguchi et al., 2006).

Hemicellulose: Hemicellulose is made of several heteropolymers (matrix polysaccharides) present in almost all plant cell walls along with cellulose (Fig. 2). While cellulose is crystalline, strong, and resistant to hydrolysis; hemicellulose has a random, amorphous structure with less strength. Hemicellulose is a polysaccharide related to cellulose and comprises 20-40% of the biomass of most plants. In contrast to cellulose, hemicellulose is derived from several sugars in addition to glucose, including especially xylose but also mannose, galactose, rhamnose and arabinose (Shambe and Kennedy, 1985). Branching in hemicellulose produces an amorphous structure that is more easily hydrolyzed than cellulose (Shaw, 2008). Also, hemicellulose can be dissolved in strong alkali solutions. Hemicellulose provides structural integrity to the cell. Some researchers believe that natural bonding may occur due to the adhesive properties of degraded hemicellulose (Bhattacharya et al., 1989).

Lignin: Lignin is a complex chemical compound most commonly derived from wood and is an integral part of the cell walls of plants (Lebo et al., 2001; Zandersons et al., 2004). The compound has several unusual properties as a biopolymer, not the least its heterogeneity in lacking a defined primary structure. Lignin fills the spaces in the cell wall between cellulose and hemicellulose (Fig. 2). It is covalently linked to hemicellulose and thereby crosslinks different plant polysaccharides, conferring mechanical strength to the cell wall and consequently to the whole plant structure (Chabannes et al., 2001).

Lignin acts as a binder for the cellulose fibres (Fig. 2). van Dam et al. (2004) have reported that lignin can be used as an intrinsic resin in binderless board production due to the fact that when lignin melts (temperatures above 140°C), it exhibits thermosetting properties. Lignin is the component that permits adhesion in the wood structure, and is a rigidifying and bulking agent (Anglès et al., 2001). Lehtikangas (2001) reported that water (8-15%) in pellets will reduce the softening temperature of lignin to 100-135°C by plasticizing the molecular chains. The adhesive properties of thermally softened lignin are thought to contribute considerably to the strength characteristics of briquettes made of lignocellulosic materials (Granada et al., 2002; Shaw, 2008).

Figure 2.

Location and arrangement of cellulose microfibrils in plant cell walls (Murphy and McCarthy, 2005; Shaw, 2008).

2.2. Rapid characterization of lignocellulosic materials

The effect of various pre-processing and pre-treatment methods (Fig. 1) on the lignocellulosic matrix at the molecular level is not well understood. Applications of pre-processing methods such as size reduction or increasing porosity, and pre-treatment techniques such as steam explosion on agricultural biomass have demonstrated an improvement in pellet (compact) quality that can be attributed to the changes in the lignocellulosic components and distribution (Bagby, 1982; Focher et al., 1998). Therefore, it is critical to rapidly quantify the change in cellulose, hemicelluloses and lignin components of biomass due to application of pre-treatment methods.

Infrared spectroscopy has the potential to produce qualitative and quantitative analytical data for samples with minimum or no sample preparation, and at high speed and throughput (Adapa et al., 2011b and 2009; Budevska, 2002; Luypaert et al., 2003; Smola and Urleb, 2000; Tucker et al., 2000). Traditionally, chemical analyses of the individual components (e.g., lignin) of lignocellulosics have been performed by acid hydrolysis followed by gravimetric determination of lignin (Kelley et al., 2004). These methods can provide highly precise data. However, these methods are laborious, time-consuming, and, consequently, expensive to perform and sample throughput is limited.

2.3. Fourier transform infrared spectroscopy

Fourier Transform Infrared Spectroscopy (FTIR) can be used to rapidly characterize and quantify cellulose-hemicellulose-lignin composition prior to and after application of various methods of pre-processing and pre-treatment of biomass (Adapa et al., 2009). The quantitative analysis of FTIR absorption spectrometry is based on the Bouguer-Beer-Lambert law (Sherman Hsu, 1997). According to this law, the intensities of absorption bands are linearly proportional to the concentration of each component in a homogenous mixture or solution.

Regression equations to predict the lignocellulosic content of agricultural biomass can be developed using pure cellulose, hemicelluloses and lignin as reference samples, and subsequently mixing them in different proportions to determine the change in absorption intensity at characteristic peak height (Adapa et al., 2011b). An overview of the experimental procedure to characterize the lignocellulosic composition is provided in Figure 3.

Pure cellulose has five distinct characteristic/ prominent peaks at wavenumbers of 1431, 1373, 1338, 1319 and 1203 cm-1. Similarly, hemicellulose (xylan) has prominent peaks at wavenumbers of 1606, 1461, 1251, 1213, 1166 and 1050 cm-1. The lignin spectrum has characteristic peaks at wavenumber of 1599, 1511, 1467, 1429, 1157 and 1054 cm-1. The intensity of absorption at characteristic peak heights of cellulose, hemicellulose and lignin were used to develop regression equations to predict lignocellulosic composition of any agricultural biomass (Table 1) (Adapa et al., 2011b).

Figure 3.

Experimental procedure followed to characterize lignocellulosic composition of agricultural straw (Adapa et al., 2011b).

Equation % Mean Absolute Deviation
% C e l l u l o s e = - 135.10 + 781.35 P H _ 1319 - 795.57 P H _ 1431 - 135.26 P H _ 1203 + 436.11 P H _ 1338 - 94.24 P H _ 1373 7.5
% H e m i c e l l u l o s e = 1638.72 - 2581.71 P H _ 1251 × P H _ 1461 - 1260.90 P H _ 1213 - 2518.05 P H _ 1166 + 1573.69 P H _ 1213 × P H _ 1251 + 118.74 P H _ 1050 + 3128.51 P H _ 1166 × 1251 + 2179.65 P H _ 1461 + 92.36 P H _ 1606 - 2294.15 P H _ 1251 - 59.29 P H _ 1461 × P H _ 1606 2.5
% L i g n i n = 7110.87 + 388.32 P H _ 1511 × P H _ 1599 - 16440.93 P H _ 1467 + 447.36 P H _ 1599 2 + 19572.82 P H _ 1157 × P H _ 1467 + 18374.36 P H _ 1157 + 15659.98 P H _ 1054 × P H _ 1429 - 4952.80 P H _ 1157 × P H _ 1599 + 800.20 P H _ 1511 - 3032.75 P H _ 1429 2 - 11269.16 P H _ 1429 - 948.04 P H _ 1511 2 + 3444.69 P H _ 1599 - 12344.90 P H _ 1054 - 16689.44 P H _ 1157 2 3.8
Note: PH – Characteristic Peak Height (Photoacoustic Units)

Table 1.

Regression equations to predict the lignocellulosic composition of agricultural biomass (Adapa et al., 2011b).

Advertisement

3. Pre-treatment of lignocellulosic biomass

3.1. Need for pre-treatment

Upon densification, many agricultural biomass materials, especially those from straw and stover, result in a poorly formed pellets or compacts that are more often dusty, difficult to handle and costly to manufacture. This is caused by lack of complete understanding on the natural binding characteristics of the components that make up biomass (Sokhansanj et al., 2005). The natural binding characteristics of lignocellulosic biomass can be enhanced by modifying the structure of cellulose-hemicellulose-lignin matrix by application of pre-processing and pre-treatment methods (Sokhansanj et al. 2005). It is postulated that by disrupting the lignocellulosic matrix of biomass materials via application of various chemical, physico-chemical (steam explosion, microwave, and radio frequency heating), and biological pre-treatment, the compression and compaction characteristics can be improved (Shaw 2008; Kashaninejad and Tabil, 2011). When high molecular amorphous polysaccharides are reduced to low molecular components, the polymer becomes more cohesive in the presence of moisture (Chen et al., 2004). The cellulose-hemicellulose-lignin matrix can be broken down to smaller amorphous molecules through acid or alkaline hydrolysis as well as through steam explosion (Ladisch, 1989; Vlasenko, 1997). Alkaline or acid solutions are often used for pre-treatment of biomass and the effect of pre-treatment depends on the lignin content of biomass. When biomass is treated with dilute alkaline solution, the internal surface area of the material is increased by swelling. Swelling causes a decrease in the degree of polymerization, separation of structural linkages between lignin and carbohydrates and disruption of the lignin structure (Fan et al., 1987). Increased moisture content resulting from chemical and enzymatic treatments is a problem, as the treated biomass has to be dried prior to densification. Steam explosion results in the hemicelluloses being hydrolyzed and water soluble, the cellulose is slightly depolymerized, the lignin melts and is depolymerized, which aid in binding particles together during densification. Zandersons et al. (2004) stated that activation of lignin and changes in the cellulosic structure during the steam explosion process facilitate the formation of new chemical bonds. Lam et al. (2008) reported that the quality (durability) of compacts produced from steam exploded sawdust was 20% higher than non-treated sawdust.

3.2. Physico-chemical pre-treatments

3.2.1. Steam explosion

Steam explosion is one of the most applied pre-treatment processes owing to its low use of chemicals and limited energy consumption (Harmsen et al., 2010). During steam explosion pre-treatment process, the lignocellulosic biomass is heated with high pressure saturated steam having temperatures typically in the range of 180-230°C for 2-10 minutes. Subsequently, the substrate is quickly flashed to atmospheric pressure; as a result, the water inside the substrate vaporizes and expands rapidly, disintegrating the biomass (Grous et al., 1985; Kokta and Ahmed, 1998; Zimbardi et al., 1999). This causes great reduction in the particle size of the substrate (Fig. 4). The heart of the explosion pulping process is the reactor, which allows the use of high pressure during heating and cooking. The reactor can be of either the batch (Fig. 5) (Jin and Chen, 2006) or continuous type (Fig. 6) (Kokta and Ahmed, 1998; Adapa et al., 2010a).

Figure 4.

Photographs showing the non-treated (30 mm hammer mill screen size) and steam exploded barley, canola, oat and wheat straw grinds.

The extent of chemical and structural modifications from steam-explosion pre-treatment depends on residence time, temperature, particle size and moisture content (Sun and Cheng, 2002). However, the severity (Ro) of steam explosion is quantified as a function of retention time and reaction temperature (Equation 1) (Overend and Chornet, 1987; Viola et al. 2008).

R o = t × e x p T - 100 14.75 E1

Where T is the temperature in °C and t is the time in minutes.

According to Zimbardi et al. (1999), the simplest way to carry out steam explosion is by batch procedure, hence widely reported in literature. However, the continuous reactors are of major interest for industrial applications. They have indicated that although the products obtained at the same treatment, severity in batch and continuous reactors are macroscopically different at first sight, there is still a lack of understanding to explain these differences. Consequently, they have developed experimental relationships between the two systems useful in making the data transfer straightforward (Equation 2).

l o g R o B a t c h = 1.50 × l o g R o C o n t i n u o u s - 1 E2

In addition, studies have been carried out to try to improve the results of steam explosion by addition of chemicals such as acid or alkali (Cara et al., 2008; Harmsen et al., 2010; Stenberg et al., 1998; Zimbardi et al., 2007). Limitations of steam explosion include the formation of degradation products that may inhibit downstream processes (Garcia-Aparicio et al., 2006).

Figure 5.

Schematic diagram of the FJM-200 fluidized bed opposed jet mill. 1, Infeed; 2, collection; 3, classification section; 4, grinding section; 5, compressed air; 6, discharge opening (Jin and Chen, 2006).

Figure 6.

The Andritz (ANDRITZ AG, Graz, Austria) continuous biomass steam explosion facility for manufacturing of Medium Density and High Density Fiberboards (MDF/HDF), Forintek pilot plant at the FPInnovations, Quebec City, Quebec (Adapa et al., 2010a).

3.2.2. Microwave and radio frequency (RF) heating

Dielectric heating is an alternative method to conventional heating. Unlike conduction/convection heating, which is based on superficial heat transfer, dielectric heating is based on volumetric and rapid heat transfer (de la Hoz et al., 2005). When lignocellulosic materials are placed in an electric field for dielectric heating pre-treatment, dipole molecules such as water or other dielectric materials, rotate vigorously to orient in the field. More polar components will absorb more energy, and thus, “hot spots” will be created in non-homogeneous materials. It is hypothesized that this unique heating feature results in an “explosion” effect in the particles and improves the disruption of the lignocellulosic structures. In addition, the non thermal effects of electromagnetic field accelerate the disintegration of the crystal structures (de la Hoz et al., 2005). Dielectric heating can be categorized as microwave or radio frequency depending on the wavelength used in the heating devices (Oberndorfer et al., 2000).

Microwave is electromagnetic waves between 300 MHz (wavelength 1 m) and 300 GHz (wavelength 1 mm). This range of spectrum lies between infrared and radio frequency radiation. Microwave irradiation has been extensively used in many processes because of its high heating efficiency and easy operation. Microwave energy can penetrate into materials and heat them quickly and uniformly. Microwave irradiation is considered to create thermal and non thermal effects. It has been applied as an efficient pre-treatment technique to enhance the hydrolysis of biomass materials. Some studies have demonstrated that microwave irradiation can change the structure of lignocellulosic materials and degrade or reduce lignin content, reduce cellulose crystallinity, and increase porosity and surface area of the materials (Azuma, 1984; Zhu et al., 2006b; Kashaninejad and Tabil, 2011).

This pre-treatment involves microwave irradiation of immersed biomass in an aqueous environment. Different types of lignocellulosic materials have been pre-treated using microwave irradiation including wheat straw (Ooshima et al., 1984; Zhu et al., 2006b; 2006c; Kashaninejad and Tabil, 2011), barley straw (Kashaninejad and Tabil, 2011), rice straw (Ooshima et al., 1984; Zhu et al., 2005 ; 2006a), rice hulls (Magara and Azuma, 1989), sugarcane bagasse (Ooshima et al., 1984; Magara and Azuma, 1989; Kitchaiya et al., 2003), switchgrass (Hu and Wen, 2008; Keshwani et al., 2007) and woody materials (Azuma et al., 1984). These materials were subjected to microwave pre-treatment of 2450 MHz in the range of 250 to 1000 W. The temperature of operation ranged from 70 to 230˚C, while heating time varied from 5 to 120 minutes. However, higher microwave power with short pre-treatment time and the lower microwave power with long pre-treatment time had almost the same effect on chemical composition of lignocellulosic materials (Zhu et al., 2005; 2006b; Kashaninejad and Tabil, 2011).

In order to increase the efficiency of microwave heating pre-treatment, some researchers have combined microwave treatment with alkaline treatment such as NaOH or Ca(OH)2. Some used alkaline solution during microwave heating treatment (Zhu et al., 2005; 2006a; 2006b; 2006c; Keshwani et al., 2007; Kashaninejad and Tabil, 2011) and some applied the alkaline solution before the lignocellulosic materials were subjected to microwave irradiation (Zhu et al., 2006a; Hu and Wen, 2008). Combination of microwave irradiation and alkali treatment improves the degradation of biomass by accelerating the reactions during the pre-treatment process compared with the conventional heating chemical pre-treatment process. Remarkable changes (Table 2) have been reported in the chemical composition of biomass samples after microwave-alkali pre-treatment, particularly in hemicellulose, lignin, and cellulose contents (Kashaninejad and Tabil, 2011). It has been reported that alkali treatment dissolves lignin and hemicellulose, and microwave irradiation facilitates dissolving these components in alkali solutions (Jackson, 1977; Kumar et al., 2009; Lesoing et al., 1980; Zhu et al., 2005). Biomass samples pretreated by microwave-alkali technique have lower lignin, hemicellulose, and cellulose than samples pretreated by microwave-distilled water or untreated samples. Moreover, degradation and depolymerisation of lignin to smaller phenolic components is another influence of microwave-alkali pre-treatment that could be considered as binder in densification process. The pellets made from microwave-chemical pre-treated biomass grinds have significantly higher density and tensile strength (Table 3) than the untreated or samples pre-treated by microwave alone (Kashaninejad and Tabil, 2011).

Radio frequency (RF) can penetrate more deeply into the materials compared with microwave heating because the radio frequency wavelength is up to 360 times greater than microwave (Marra et al., 2007). This unique characteristic is an advantage to treat large amount of material and it is easier to scale up the process. While radio frequency as a heating method has been widely applied in food-processing industries, there is not much report on application of radio frequency heating for lignocellulosic materials pre-treatment. Hu et al. (2008) used radio frequency heating in the NaOH pre-treatment of switchgrass to enhance its enzymatic digestibility. Because of the unique features of radio frequency heating (i.e., volumetric heat transfer, deep heat penetration of the samples, etc.), switchgrass could be treated on a large scale, at high solids content, and with a uniform temperature profile. At 20% solids content, radio frequency-assisted alkali pre-treatment (at 0.1 g of NaOH/g of biomass loading and 90°C) resulted in a higher xylose yield than the conventional heating pre-treatment. The optimal particle size and alkali loading in the radio frequency pre-treatment were determined to be 0.25-0.50 mm and 0.25 g of NaOH/g of biomass, respectively.

Treatment Wheat straw Barley straw
Protein Lignin Ash Starch Cellulose Hemicellulose Protein Lignin Ash Starch Cellulose Hemicellulose
Untreated 1.99b 8.33a 6.33f 1.11d 44.99b 27.96a 1.61d 11.95a 6.03d 0.79c 46.93a 27.40a
Microwave-distilled water 2.24a 8.01c 8.87e 1.48b 39.69d 22.62b 2.01a 8.85b 6.28d 1.08b 45.25b 27.21a
Microwave-NaOH (1%) 1.41e 7.82d 17.32b 1.89a 35.82e 12.32d 1.80b 6.65e 16.96b 0.60e 40.81c 8.74c
Microwave-NaOH (2%) 1.36f 7.09f 34.77a 0.27f 34.77f 4.06f 1.62d 4.52f 41.43a 0.54f 35.22d 5.46d
Microwave-Ca(OH)2 (1%) 1.85c 8.11b 12.24d 0.69e 45.66a 14.94c 1.81b 7.27d 13.21c 0.72d 41.01c 15.00b
Microwave-Ca(OH)2 (2%) 1.52d 7.55e 15.89c 1.31c 42.56c 11.10e 1.68c 8.16c 16.73b 1.19a 41.24c 8.97c
Means with the same letters designation (a, b, c, d, and e) in a column are not significantly different at P = 0.05.

Table 2.

Chemical composition (% dry basis) of untreated and microwave pretreated of wheat and barley straw at power 713 W.

Treatment Wheat straw Barley straw
Fracture load (N) Tensile strength (MPa) Fracture load (N) Tensile strength (MPa)
Untreated 19.10±5.61 0.81±0.24 16.25±5.30 0.68±0.22
Microwave- distilled water 35.00±11.93 1.48±0.46 14.25±5.31 0.61±0.21
Microwave- NaOH (1%) 85.46±22.94 3.99±0.82 57.13±12.12 2.42±0.47
Microwave- NaOH (2%) 88.00±15.86 3.69±0.66 90.75±22.42 3.59±0.98
Microwave- Ca(OH)2 (1%) 67.05±19.82 3.03±0.79 42.38±10.30 1.83±0.49
Microwave- Ca(OH)2 (2%) 78.25±25.07 3.31±1.03 67.25±19.94 2.88±0.91

Table 3.

Effect of microwave-chemical pre-treatments on fracture load and tensile strength of wheat and barley straw pellets at power 713 W.

3.2.3. Chemical pre-treatment

Different chemicals such as acids, alkalis, oxidizing agents and ozone have been used for chemical pre-treatment of lignocellulosic materials. Depending on the type of chemical used, pre-treatment could have different effects on structural components. Alkaline pre-treatment, ozonolysis, peroxide and wet oxidation pre-treatments were reportedly more effective in lignin removal, whereas dilute acid pre-treatment was more efficient in hemicellulose solubilization (Galbe and Zacchi, 2002; Sánchez and Cardona, 2008; Tomas-Pejo et al., 2008).

Acid Hydrolysis: Inorganic acids such as H2SO4 and HCl have been used for pre-treatment of lignocellulosic materials and have been used on a wide range of feedstocks ranging from hardwoods to grasses and agricultural residues. Acid hydrolysis can be classified as concentrated or dilute-acid hydrolysis based on the dose of acid used in the process. In the first case, the biomass is treated with high concentration of acids at ambient temperatures, which results in high conversion of lignocellulosic materials. Although concentrated acids are powerful agents for cellulose hydrolysis, they are toxic, corrosive, hazardous, and thus require reactors that are resistant to corrosion, making the pre-treatment process very expensive. In addition, the concentrated acid must be recovered after hydrolysis to make the process economically feasible (Galbe and Zacchi, 2002; Sun and Cheng, 2002).

Dilute-acid hydrolysis has been successfully developed for pre-treatment of lignocellulosic materials. Sulfuric acid at concentrations usually below 4% (wt) has been of the most interest in such studies as it is inexpensive and effective. Dilute H2SO4 pre-treatment can achieve high reaction rates and significantly improve cellulose hydrolysis (Esteghlalian et al., 1997). High temperature is favorable to attain acceptable rates of cellulose conversion. Despite low acid concentration and short reaction time, the use of high temperatures in dilute-acid hydrolysis accelerates the rate of hemicellulose sugar decomposition and increases equipment corrosion (Galbe and Zacchi, 2002; Taherzadeh and Karimi, 2007).

Alkali hydrolysis: Dilute alkali such as sodium, potassium, calcium, and ammonium hydroxides have been used for pre-treatment of lignocellulosic materials in alkali hydrolysis. The effectiveness of these agents depends on the lignin content of the materials. Temperature and pressure are lower in alkali pre-treatment compared with other pre-treatment methods (Mosier et al., 2005). Alkali pre-treatment can be conducted at ambient conditions, but process time is longer (hours or days instead of minutes or seconds). Compared with acid process, alkaline process causes less sugar degradation, and many of the caustic salts can be recovered and/or regenerated.

Sodium hydroxide has been studied more than other agents (Soto et al., 1994; Fox et al., 1989; MacDonald et al., 1983). Treatment of lignocellulosic materials using dilute NaOH results in swelling, leading to an increase in internal surface area, a decrease in the degree of polymerization, a decrease in crystallinity, separation of structural linkages between lignin and carbohydrates, and disruption of the lignin structure. However, calcium hydroxide (lime) is the least expensive hydroxide and has been shown to be an effective pre-treatment agent. The process of lime pre-treatment involves slurrying the lime with water, spraying it onto the biomass material, and storing the material in a pile for a period of hours to weeks. The particle size of the biomass is typically 10 mm or less. Elevated temperatures reduce contact time.

Oxidizing agents: In this pre-treatment, an oxidizing compound such as hydrogen peroxide (H2O2) or peracetic acid (CH3CO3H) is used to treat lignocellulosic materials and sometimes is applied in combination of an alkaline solution (e.g. NaOH) to improve effectiveness. This pre-treatment is usually carried out under mild temperature. This pre-treatment is more effective to increase crop residue digestibility compared with NaOH pre-treatment alone. Gould (1984) delignified agricultural residues using 1% H2O2 at 25°C for 18–24 h. Under this condition, more than half of the lignin and most of hemicellulose were solubilized. The pre-treatment of cane bagasse with H2O2 greatly enhanced its susceptibility to further hydrolysis. About 50% of the lignin and most of the hemicellulose were solubilized by 2% H2O2 at 30°C within 8 h, and a 95% efficiency of glucose production from cellulose was achieved in the subsequent saccharification by cellulase at 45°C for 24 h (Azzam, 1989).

Ozonolysis: In this process, ozone is used to change the structure of lignocellulosic materials and has been used for different materials such as wheat straw (Ben-Ghedalia and Miron, 1981), bagasse, green hay, peanut, pine ( Neely, 1984), cotton straw (Ben-Ghedalia and Shefet, 1983) and poplar sawdust (Vidal and Molinier, 1988). Ozonolysis is carried out at room temperature and normal pressure. It can effectively remove the lignin without producing any toxic residues. In this process, hemicellulose is slightly affected, but no change in cellulose has been reported. The main restriction of this process is the large amount of ozone utilization that makes the process expensive (Sun and Cheng, 2002). Binder et al. (1980) reported 60% removal of the lignin from wheat straw using ozone pre-treatment. Enzymatic hydrolysis yield increased from 0% to 57% as the percentage of lignin decreased from 29% to 8% after ozonolysis pre-treatment of poplar sawdust (Vidal and Molinier, 1988). Garcia-Cubero et al. (2009) studied the ozonolysis pre-treatment of wheat straw in a fixed bed reactor at room conditions and concluded that enzymatic hydrolysis yield of up to 88.6% compared to 29% in non-ozonated sample.

3.3. Biological pre-treatment

Most pre-treatments require expensive instruments or equipment that require high energy requirements, depending on the process. In particular, physical and thermo-chemical processes require ample amount of energy to change the lignocellulosic structure of biomass. Biological pre-treatment using various types of rot fungi is a process that does not require high energy for lignin removal from a lignocellulosic biomass, despite extensive lignin degradation. Biological pre-treatments are safe, environmentally friendly and less energy intensive compared to other pre-treatment methods. However, the rate of hydrolysis reaction is very slow and needs a great improvement to be commercially applicable.

Biological pre-treatment comprises of using microorganisms such as brown-, white-, and soft-rot fungi for selective degradation of lignin and hemicellulose among which white-rot fungi seems to be the most effective microorganism (Fan et al., 1987). Brown rots mainly attack cellulose, while white and soft rots attack both cellulose and lignin. Lignin degradation occurs through the action of lignin-degrading enzymes such as peroxidases and laccase (Okano et al., 2005). These enzymes are regulated by carbon and nitrogen sources. The suitable fungi for biological pre-treatment should have higher affinity for lignin and degrade it faster than carbohydrate components.

Hatakka et al. (1983) studied the pre-treatment of wheat straw by 19 white-rot fungi and found that 35% of the straw was converted to reducing sugars by Pleurotus ostreatus in 5 weeks. Similar conversion was obtained in the pre-treatment by Phanerochaete sordid (Ballesteros et al., 2006) and Pycnoporus cinnabarinus (Okano et al., 2005) in 4 weeks. Akin et al. (1995) also reported the delignification of bermudagrass by white-rot fungi. The biodegradation of bermudagrass stems was improved by 29-32%, after 6 weeks, using Ceriporiopsis subvermispora and by 63-77% using Cyathus stercoreus.

Advertisement

4. Particle size reduction and physical properties

The application of pre-processing operations such as particle size reduction/ grinding is critical in order to increase the surface area of lignocellulosic biomass prior to densification (Mani et al. 2003). Particle size reduction increases the total surface area, pore size of the material and the number of contact points for inter-particle bonding in the compaction process (Drzymala, 1993). Size reduction is an important energy intensive unit operation essential for bioenergy conversion process and densification to reduce transportation costs (Bitra et al., 2009; Soucek et al., 2003). Energy consumption of grinding biomass depends on initial particle size, moisture content, material properties, feed rate of the material and machine variables (Lopo, 2002). A comprehensive summary of literature review on size reduction of lignocellulosic biomass is provided in Table 4.

Type of Choppers/ Grinders Biomass Parameters Measured and Correlations Observations Reference
Hammer Mill Non-Treated and Steam Exploded Barley, Canola, Oat and Wheat Straw Hammer mill screen size (from 1.6 to 30.0 mm) on Specific Energy
Effect of geometric mean particle size on bulk density
Effect of geometric mean particle size on particle density
Analysis on ground particle size distribution
Negative exponential and power correlation between geometric mean particle size with both bulk and particle density
Specific energy requirement is material dependent
Negative power correlation between hammer mill screen size and specific energy
Shapiro-Wilk Test for normality was performed
Adapa et al., 2011a
Tub Grinder Rectangular Wheat Straw Bales, Round Rice Straw and Corn Stover Bales Effect of screen sizes (from 12.7 to 50.8 mm) on Specific Energy
Effect of screen sizes on grinding rate
Analysis on ground particle size distribution
Positive correlation between screen size and grinding rate
Positive correlation between tub rotational speed and grinding rate
Specific Energy is material dependent
Negative power/ exponential correlation between screen size and specific energy
Arthur et al., 1982
Hammer Mill Coastal Bermudagrass Effect of moisture content on Specific Energy
Effect of feed rate on Specific Energy
Positive correlation between moisture content and specific energy
Positive correlation between feed rate and specific energy
Balk, 1964
Hammer Mill Wheat Straw and Corn Stover Effect of operating speeds (from 2000 to 3600 rpm) on Specific Energy
Effect of hammer angles (90° and 30° hammers) on Specific Energy
Analysis on ground particle size distribution
Positive correlation between operating speed and specific energy
Geometric mean particle diameter decreased with an increase in hammer mill speed
Specific energy increased with a decrease in hammer angle
Bitra et al., 2009
Knife and Hammer Mills Hardwood Chips, Wheat Straw and Corn Stover Effect of screen size (from 1.6 to 12.7 mm) on specific energy Negative correlation between screen size and specific energy
Specific Energy is material dependent
Cadoche and López, 1989
Hammer Mill Red Winter Wheat Straw Effect of screen size (from 1.59 to 4.76 mm) on specific energy
Effect of feed rate (from 1.5 to 2.5 kg/min) on specific energy
Negative correlation was observed between screen size and specific energy
Feed rate did not have significant effect on specific energy
Fang et al., 1997
Hammer Mill Wheat Straw Effect of screen size (3.2 and 1.6 mm) on Specific Energy
Analysis on ground particle size distribution
Negative correlation between specific energy and screen size Himmel et al., 1985
Tub Grinders Round Bales of Corn Stover and Perennial Grasses Effect of screen size (from 19.1 to 127.0 mm) on Specific Energy
Effect of screen size on throughput
Effect of screen size on bulk and particle densities
Negative correlation between screen size and bulk density
Positive correlation between screen size and particle density
Negative correlation between screen size and specific energy
Positive correlation between screen size and throughput
Kaliyan et al., 2010
Hammer Mill Barley Straw, Corn Stover and Switchgrass Effect of Screen Sizes (3.2, 1.6 and 0.8 mm) on Specific Energy
Effect of Moisture Content (8% and 12% wb) on Specific Energy
Correlation between bulk and particle densities and geometric mean diameter
Analysis on ground particle size distribution
Negative linear correlation between specific energy and hammer mill screen size at 8% mc
Quadratic correlation between specific energy and hammer mill screen size at 12% mc
Polynomial relations for bulk and particle densities with geometric mean particle diameters
Mani et al., 2004
Hammer Mill Oat Straw, Rattle Grass and Miscanthus Effect of Screen size (from 1.0 to 10.0 mm) on specific energy
Effect of moisture content on specific energy
Negative power correlation between screen size and specific energy
Positive correlation between moisture content and specific energy; significantly higher specific energy is required at smaller screen sizes
Soucek et al., 2003
Hammer Mill Corn Stover Effect of hammer thickness (6.4 and 3.2 mm) on Specific Energy
Effect of hammer thickness (6.4 and 3.2 mm) on Grinding Rate
Effect of hammer tip speed (54 to 86 m/s) on Specific Energy
Negative correlation between hammer thickness and Specific Energy
Negative correlation between hammer thickness and Grinding Rate
Positive correlation between hammer tip speed and Specific Energy
Vigneault et al., 1992
Knife Mill Switchgrass, Corn Stover, and Wheat Straw Effect of rotational speed (from 250 to 500 rpm) on specific energy
Analysis on ground particle size distribution
Positive correlation between rotational speed and specific energy
Screen size has significant effect on particle size distribution
Womac et al., 2007

Table 4.

A comprehensive summary of literature review on size reduction of lignocellulosic biomass.

4.1. Chopping

Baled agricultural biomass from the field does not have good flowing characteristics and may not flow easily into grinders such as hammer mills and disc refiners. Therefore, biomass needs to be chopped with a chopper (rotary shear shredder)/ knife mill/ tub grinder to accommodate bulk flow and uniformity of feed rate. A chopper, knife cutter, or knife mill is often used for coarse size reduction (>50 mm) of stalk, straw, and grass feed stocks (Bitra et al., 2009). Knife mills reportedly worked successfully for shredding forages under various crop and machine conditions (Cadoche and López, 1989).

Bitra et al. (2009) reported that the total specific energy (including energy to operate the knife mill) for agricultural biomass chopping increases with knife mill speed. The total specific energy for knife mill and tub grinder has been observed to have negative correlation with screen size and mass feed rate (Arthur et al., 1982; Bitra et al., 2009; Himmel et al., 1985). However, grinding rate (throughput) increases with an increase in screen size (Arthur et al., 1982).

For tub grinders, an increase in screen size results in an increase in geometric mean length of particles and throughput, but a decrease in bulk density of the particles and specific energy consumption (Kaliyan et al., 2010).

4.2. Hammer mill grinding

Typically, hammer mills are used in forage processing industry as they are relatively inexpensive, easy to operate and produces wide range of particles (Lopo, 2002). Hammer mills have achieved merit because of their ability to finely grind a greater variety of materials than any other machines (Scholten et al., 1985). The performance of a hammer mill is measured in terms of energy consumption and geometric mean diameter and particle size distribution of the ground product (Adapa et al., 2011a; Mani et al., 2004).

Screen Size: Hammer mill screen opening size was the most significant factor affecting mill performance (Fang et al., 1997) and also has significant effect on mean particle size (Pfost and Headley, 1971). The specific energy required to grind agricultural biomass significantly increases with a decrease in hammer mill screen size and shows a negative power correlation (Arthur et al., 1982; Soucek et al., 2003). Similarly, Adapa et al. (2011a) reported negative correlation between specific energy and particle size of biomass as affected by hammer mill screen sizes. However, two other studies reported a second-order polynomial relationship between the specific energy requirements for grinding biomass (Mani et al. 2004; Sitkei, 1986). Usually, the mean geometric particle size for any particular biomass decreases with a decrease in hammer mill screen size (Adapa et al., 2011a). It has been reported that wider particle size distribution is suitable for compaction (pelleting/ briquetting) process (Adapa et al., 2011a; Mani et al., 2004). During compaction, smaller (fine) particles rearrange and fill in the void space of larger (coarse) particles producing denser and durable compacts (Tabil, 1996).

Operating Speed (Peripheral Velocity): The speed has a significant effect on mean particle size (Pfost and Headley, 1971). The total specific energy of hammer mill grinding has direct correlation to an increase in hammer tip speed (Bitra et al., 2009; Vigneault et al., 1992). High speed hammer mills with smaller diameter rotors are good for fine or hard-to-grind material. However, at high tip speeds, the material moves around the mill parallel to the screen surface making the openings only partially effective. At slower speeds, the material impinges on the screen at a greater angle causing greater amounts of coarser feed to pass through (Balk, 1964).

Hammer Angles and Thickness: The direct energy input for grinding also depends on hammer angles. In general, the specific energy for grinding decreases with an increase in hammer degrees (Bitra et al., 2009). In addition, the specific energy for grinding increases with an increase in hammer thickness (Vigneault et al., 1992).

Material Moisture Content and Feed Rate: A positive correlation has been reported between moisture content and specific energy consumption for grinding of agricultural biomass (Balk, 1964; Mani et al., 2004; Soucek et al., 2003). Feeding rate also has significant effect on specific energy consumption during hammer mill grinding and has positive correlation (O’Dogherty, 1982).

Bulk and Particle Densities, and Geometric Mean Particle Size: Usually, the bulk and particle density of agricultural straw significantly increases with a decrease in hammer mill screen size (Adapa et al., 2011a). The geometric mean particle size of pre-treated straw is usually smaller than that of the non-treated straw. This could be due to the fact that application of pre-treatment disrupts/ disintegrates the lignocellulosic structure of the biomass (Sokhansanj et al., 2005) leading to lower shear strength (easier to grind the straw).

4.3. Physical and frictional properties of biomass

Bulk Density: The goal of densification is to increase the bulk density of agricultural straw to facilitate economic storage, transportation and handling of the material. In addition, densification results in an increase in the net calorific content per unit volume. The bulk density of agricultural biomass depends on the type of biomass, moisture content, grind size, and pre-treatment (Mani et al., 2006). Lower bulk densities, and concerns with uneven and low flowability of straw grinds are critical issues to sustainable production of pellets using pellet mills (Adapa et al., 2009; Larsson et al., 2008).

Typically, the bulk density of ground straw increases with a decrease in hammer mill screen size. Also, pre-treatments usually results in a decrease in bulk density since the organized lignocellulosic structure of biomass is disturbed/ disintegrated. In addition, the bulk density and geometric mean particle size of material is correlated by either power or exponential relations (Adapa et al., 2010b; Mani et al., 2004). Table 5 shows a summary of average bulk density of various agricultural biomasses ground using a hammer mill.

Particle Density: Particle size of the grinds will have direct effect on the final pellet density. Theoretically, the density of pellet can be as high as the particle density of the ground biomass. Similar to bulk density, particle density also depends on the type of biomass, moisture content, grind size, and pre-treatment (Adapa et al., 2010b). The particle density is observed to have negative correlation with hammer mill screen size. Application of pre-treatment increases the particle density since disturbance/ disintegration of lignocellulosic structure results in finer components (Adapa et al., 2010b). Table 5 shows a summary of average particle density of various agricultural biomasses ground using a hammer mill.

Geometric Mean Particle Size and Distribution: It has been reported that wider particle size distribution is suitable for compaction (pelleting/briquetting) process (Mani et al., 2004a). During compaction, smaller (fine) particles rearrange and fill in the void space of larger (coarse) particles producing denser and durable compacts (Tabil, 1996). Therefore, ideally the grinds should be normally distributed, should have near zero skewness and lower peak than expected for the normal and wider distribution of data (negative Kurtosis values). In addition, a decrease in the biomass grind size has been observed to have a positive effect on pellet mill throughput (Adapa et al., 2004).

Frictional Properties: Prior to densification, biomass grinds need to be efficiently stored, handled and transported. Physical and frictional properties of biomass have significant effect on design of new and modification of existing bins, hoppers and feeders (Fasina et al., 2006). The frictional behavior of biomass grinds in all engineering applications is described by two independent parameters: the coefficient of internal friction, and the coefficient of wall friction. The former determines the stress distribution within particles undergoing strain, and the latter describes the magnitude of the stresses between the particle and the walls of its container (Seville et al., 1997). The classic law of friction states that frictional force is directly proportional to the total force that acts normal to the shear surfaces (Chancellor, 1994; Chung and Verma, 1989; Larsson, 2010). Frictional force depends on the nature of the materials in contact but is independent of the area of contact or sliding velocity (Mohsenin, 1970). Material properties such as moisture content and particle size affect the frictional properties and densification performance of an individual feedstock (Larsson 2010; Shaw and Tabil, 2006). In addition, the determination of coefficient of friction is essential for the design of production and handling equipment and in storage structures (Adapa et al., 2010a; Puchalski and Brusewitz, 1996). A comprehensive summary of literature review on coefficient of internal friction and cohesion of agricultural biomass is provided in Table 6.

Predominantly, a linear correlation exists between normal and shear stress for agricultural straw grinds (Adapa et al., 2010a; Chevanan et al., 2008; Richter, 1954) at any specific hammer mill screen size. An increase in hammer mill screen size significantly decreases the shear stress for ground straw at any specific normal stress (Adapa et al., 2010a).

The correlation for coefficient of internal friction and cohesion with average geometric mean particle sizes for agricultural straw grinds is provided in Adapa et al. (2010a). These correlations can be used to predict the coefficient of internal friction (slope of the linear plot) and the cohesion (intercept of the linear plot) for various geometric mean particle sizes. In general, the coefficient of internal friction for ground agricultural straw decreases with an increase in average geometric mean particle diameter. The coefficient of cohesion for straw grinds increases with an increase in average geometric mean particle size (Adapa et al., 2010a).

Biomass Hammer Mill Screen Size (mm) Moisture Content (%, wb) Geometric Mean Particle Diameter (mm) Bulk Density (kg/m3) Particle Density (kg/m3) Reference
Barley 6.4 8.9 0.88 96 1046 Adapa et al., 2011a
3.2 5.3 0.46 149 1089
1.6 7.8 0.46 155 1149
Canola 6.4 12.6 0.89 144 1019 Adapa et al., 2011a
3.2 9.2 0.52 190 1192
1.6 8.3 0.37 203 1309
Corn Stover 3.2 6.22 0.41 131 1170 Mani et al., 2004
1.6 6.22 0.26 156 1330
0.8 6.22 0.19 158 1340
Oat 6.4 10.9 0.94 111 873 Adapa et al., 2011a
3.2 9.4 0.57 156 1093
1.6 7.7 0.40 196 1240
Wheat 6.4 9.5 0.99 107 1078 Adapa et al., 2011a
3.2 9.5 0.72 141 1225
1.6 8.6 0.45 154 1269

Table 5.

Average bulk and particle densities of various agricultural biomasses ground using a hammer mill

Biomass Experimental Conditions Observations Reference
Corn Stover Normal stress from 10 to 200 kPa
Hammer mill screen sizes of 6.35 and 3.18 mm
Moisture contents of 7, 11 and 15% (wb)
Galvanized steel
Coefficient of wall friction increased from 0.18 to 0.26 with an increase in moisture from 7 to 15%
No clear trend observed for the adhesion coefficient
Mani et al., 2004
Peat hull, Switchgrass and Poultry Litter Consolidating stress from 1.5 to 12.0 kPa
Screen sizes from 0.79 to 3.20 mm
Ring shear test
No effect of screen size on internal friction and cohesive properties Fasina et al., 2006
Peat Moss, Wheat Straw, Oat Hulls and Flax Shives Normal stress from 10 to 400 kPa
Geometric mean particles sizes of 0.74 (peat moss), 0.65 (wheat straw), 0.47 (oat hulls) and 0.64 (flax shives) mm
Moisture content 9-10% (wb)
Mild steel surface
Coefficient of wall friction were 0.68 (peat moss), 0.45 (wheat straw), 0.39 (oat hulls), and 0.41 (flax shives)
Adhesion coefficients were 0.2635 kPa (peat moss), 10.687 kPa (wheat straw), 4.719 kPa (oat hulls), and 16.203 kPa (flax shives)
Shaw and Tabil, 2006
Alfalfa, Barley Straw, Wheat Straw and Whole Green Barley Normal stress from 200 to 735 kPa
Moisture content for alfalfa, barley straw from 12.0 to 45.7%, and for wheat straw at 10.0% and whole green barley at 51.0% (wb)
Chop size from 10 to 90 mm
Polished steel surface
Coefficient if friction on steel surface for alfalfa and barley straw increased with moisture content and was from 0.15 to 0.26, and 0.14 and 0.27, respectively
Coefficient of friction for wheat straw and whole green barley were 0.13 and 0.21, respectively
No effect of chop size on coefficient of internal friction on barley straw
Afzalinia and Roberge, 2007
Switchgrass, Wheat straw, and Corn Stover Normal stresses from 1.23 to 4.92 kPa
Chop size of 7.81 and 13.50 mm for switchgrass, 7.09 and 10.39 mm for wheat straw, 7.80 and 14.89 mm for corn stover
No effect of chop size on friction coefficients
Coefficient of internal friction varied from 0.765 to 1.586
Chevanan et al., 2008
Reed Canary Grass Normal stresses of 0.52-7.52 kPa (low) and 23-275 MPa (high)
Moisture contents from 6.7 to 17.1% (wb) for low normal stress, and 8.9 to 27.2% for high normal stress
Screen sizes of 4.0 mm
Ring shear test
High friction value of 0.6 was obtained at normal stress of 50 MPa and lower
At low normal stresses, the coefficient of kinematic wall friction (ratio of shear stress and normal stress) was positively correlated with moisture content and negatively correlated to normal stress
At high normal stresses, the coefficient of kinematic wall friction was negatively correlated to both moisture content and normal stress
Larsson, 2010
Non-Treated and Steam Exploded Barley, Canola, Oat and Wheat Straw Normal stress from 9.8 to 39.2 kPa
Moisture content of 10% (wb)
Screen size from 1.6 to 6.4 mm
No effect of screen size on shear stress values
Steam exploded straw had higher coefficient of internal friction than non-treated straw grinds
Coefficient of friction for non-treated barley, canola, oat and wheat straw were in the range of 0.505 to 0.584, 0.661 to 0.665, 0.498 to 0.590, and 0.532 to 0.591, respectively.
Coefficient of friction for steam exploded barley, canola, oat and wheat straw were in the range of 0.562 to 0.738, 0.708 to 0.841, 0.660 to 0.860, and 0.616 to 1.036, respectively
Adapa et al., 2010a

Table 6.

A comprehensive summary of literature review on coefficient of internal friction and cohesion of agricultural biomass

Advertisement

5. Summary

The current chapter has explored the effects of pre-treatment (chemical, physico-chemical, and biological) and pre-processing (size reduction) techniques on densification of agricultural straw resulting in high quality (density and durability) pellets. It has been determined that an increase in bulk density of biomass also increases the net calorific content per unit volume of pellets, and facilitates easy and economical storage, transport and handling of the biomass. Pre-treatment and pre-processing methods disintegrate the basic lignocellulosic structure of biomass, and change the relative composition of lignin, cellulose and hemicelluloses in the material. In addition, physical and frictional properties of agricultural straw are altered. The application of pre-treatments breaks the long-chain hydrogen bond in cellulose, making hemicelluloses amorphous, and loosening the lignin out of the lignocellulosic matrix, resulting in better quality (physically) pellets. During this process, the high molecular amorphous polysaccharides are reduced to low molecular components to become more cohesive in the presence of moisture during densification process. Particle size reduction increases the total surface area, pore size of the material and the number of contact points for inter-particle bonding in the compaction process.

It has been shown that the Fourier Transform Infrared Spectroscopy (FTIR) can be used to rapidly characterize and quantify cellulose-hemicellulose-lignin composition prior to and after application of various pre-processing and pre-treatment methods. Regression equations were developed to predict the lignocellulosic content of agricultural biomass using pure cellulose, hemicelluloses and lignin as reference samples.

References

  1. 1. Adapa, P.K., Tabil L.G. & Schoenau, G.J.2011aGrinding Performance and Physical Properties of Non-Treated and Steam Exploded Barley, Canola, Oat and Wheat Straw. Journal of Biomass and Bioenergy,doi:10.1016/j.biombioe.2010.10.00435,549 561
  2. 2. Adapa P. K. Tabil L. G. Schoenau G. J. Canam T. Dumonceaux T. 2011bQuantitative Analysis of Lignocellulosic Components of Non-Treated and Steam Exploded Barley, Canola, Oat and Wheat Straw using Fourier Transform Infrared Spectroscopy. The Journal of Agricultural Science and Technology, 5(7), (In-Press).
  3. 3. Adapa, P.K., Tabil L.G. & Schoenau, G.J.; 2010aPhysical and Frictional Properties of Ground Non-Treated and Steam Exploded Barley, Canola, Oat and Wheat Straw Grinds. Journal of Powder Technology,doi:10.1016/j.powtec.2010.03.038,201,230 241
  4. 4. Adapa P. K. Tabil L. G. Schoenau G. J. 2010bPelleting Characteristics of Selected Biomass with and without Steam Explosion Pre-treatment. International Journal of Agricultural and Biological Engineering, 3(3), 62 79
  5. 5. Adapa P. K. Karunakaran C. Tabil L. G. Schoenau G. J. 2009Potential Applications of Infrared and Raman Spectromicroscopy for Agricultural Biomass. Agricultural Engineering International: the CIGR Ejournal, Manuscript 1081, XI(February), 1 25
  6. 6. Adapa P. K. Schoenau G. J. Tabil L. G. Arinze E. A. Singh A. Dalai A. K. 2007Customized and value-added high quality alfalfa products- a new concept. Agricultural Engineering International: the CIGR Ejournal, Manuscript FP 07 003, IX(June), 1 28
  7. 7. Adapa P. K. Tabil L. G. Schoenau G. J. Sokhansanj S. 2004 Pelleting characteristics of fractionated sun-cured and dehydrated alfalfa grinds Applied Engineering in Agriculture ASAE Transactions, 20(6), 813 820
  8. 8. Afzalinia S. Roberge M. 2007 Physical and mechanical properties of selected forage materials Canadian Biosystems Engineering 2
  9. 9. Akin D. E. Rigsby L. L. Sethuraman A. Morrison W. H. Gamble G. R. Eriksson K. E. L. 1995 Alterations in structure, chemistry, and biodegradability of grass lignocellulose treated with the white rot fungi Ceriporiopsis subvermispora and Cyathus stercoreus. Applied Environmental Microbiology, 61, 1591 1598
  10. 10. Anglès M. N. Ferrando F. Farriol X. Salvadó J. 2001 Suitability of steam exploded residual softwood for the production of binderless panels. Effect of the pre-treatment severity and lignin addition Biomass and Bioenergy, 21, 211 224
  11. 11. Arthur J. F. Kepner R. A. Dobie J. B. Miller G. E. Parsons P. S. 1982 Tub grinder performance with crop and forest residues Transactions of the ASAE 1488 1494
  12. 12. Azuma J. I. Tanaka F. Koshijima T. 1984Enhancement of enzymatic susceptibility of lignocellulosic wastes by microwave radiation. Journal of Fermentation Technology, 62(4), 377 384
  13. 13. Azzam M. 1989Pre-treatment of cane bagasse with alkaline hydrogen peroxide for enzymatic hydrolysis of cellulose and ethanol fermentation. Journal of Environmental Science and Health, B., 24 (4), 421 433
  14. 14. Bagby M. O. 1982In International Symposium on Ethanol from Biomass. H. E. Duckworth and E. A. Thompson, eds. 561 569Winnipeg, MB: The Royal Society of Canada.
  15. 15. Balatinecz J. J. 1983The Potential of Densification in Biomass Utilization. In: W.A. Cote. ed. Biomass utilization. London: Plenum Press: 181 189p.
  16. 16. Balk W. A. 1964Energy requirements for dehydrating and pelleting coastal Bermuda grass. Transactions of the ASAE, 4, 349 341
  17. 17. Ben-Ghedalia D. Miron J. 1981 The effect of combined chemical and enzyme treatment on the saccharification and in vitro digestion rate of wheat straw Biotechnology and Bioengineering 823 831
  18. 18. Ben-Ghedalia D. Shefet G. 1983Chemical treatments for increasing the digestibility of cotton straw. Journal of Agricultural Sciences, 100, 393 400
  19. 19. Bhattacharya S. Sett S. Shrestha R. M. 1989 State of the Art for Biomass Densification Energy Sources 161 182
  20. 20. Binder A. Pelloni L. Fiechter A. 1980 Delignification of straw with ozone to enhance biodegradability Applied Microbiology and Biotechnology, 11, 1 5
  21. 21. Bitra, V.S.P., Womac, A.R., Chevanan, N., Miu, P.I., Igathinathane, C., Sokhansanj, S., & Smith, D.R.2009Direct mechanical energy measured of hammer mill comminution of switchgarss, wheat straw, and corn stover and analysis of their particle size distributions. Powder Technology, 193(2009)32 45
  22. 22. Budevska B. O. 2002Handbook of Vibrational Spectroscopy, 5 edited by J. M. Chalmers and P. R. Griffiths, New York: John Wiley and Sons: 3720-3732 p.
  23. 23. Cadoche L. López G. D. 1989 Assessment of size reduction as a preliminary step in the production of ethanol for lignocellulosic wastes. Biological Wastes 153 157
  24. 24. Cara C. Ruiz E. Ballesteros M. Manzanares P. Jose Negro. M. Castro E. 2008 Production of fuel ethanol from steam-explosion pretreated olive tree pruning Fuel 692 700
  25. 25. Chabannes, M., Ruel, K., Yoshinaga, A,. Chabbert, B., Jauneau, A., Joseleau, J.P., & Boudet, A.M.2001In situ analysis of lignins in transgenic tobacco reveals a differential impact of individual transformations on the spatial patterns of lignin deposition at the cellular and subcellular levels. Plant Journal, 28,doi:10.1046/j.1365-313X.2001.01159.x 271 282
  26. 26. Chancellor W. L. 1994Friction between soil and equipment materials. ASAE Paper 941034St. Joseph, MI.: American Society of Agricultural and Biological Engineers.
  27. 27. Chen W. Lickfield G. C. Yang C. Q. 2004 Molecular modeling of cellulose in amorphous state. Part I: model building and plastic deformation study Polymer 1063 1071
  28. 28. Chevanan N. Womac A. R. Bitra V. S. Yoder D. C. 2008 Flowability parameters for chopped switchgrass, wheat straw and corn stoverASABE Annual International Meeting, Rhode Island, Paper 084162St. Joseph, MI: American Society of Agricultural and Biological Engineers, June 29 July 2, 12 pages.
  29. 29. Chico-Santamarta L. Humphroes A. White D. Chaney K. Godwin R. J. 2009Effect of Pre- and Post-Pelletization Storage of Canola (Oilseed Rape) Straw on the Quality and Properties of Pellets. ASABE Annaul International Meeting, Grand Sierra Resort and Casino, Reno, Nevada, Paper 096105June 21 24 pages.
  30. 30. Chung J. H. Verma L. R. 1989Determination of friction coefficients of beans and peanuts. Transactions of the ASAE 32(2), 745
  31. 31. Crawford R. L. 1981 Lignin biodegradation and transformationNew York: John Wiley and Sons. 0-47105-743-6
  32. 32. de la Hoz A. Diaz-Ortiz A. Moreno A. 2005 Microwaves in organic synthesis: Thermal and non-thermal microwave effects Chemical Society Reviews 164 178
  33. 33. Deguchi S. Tsujii K. Horikoshi K. 2006 Cooking Cellulose in Hot and Compressed Water Chemical Communications 3293 3295 doi:10.1039/b605812d
  34. 34. Demirbaş A. 2001Biomass Resource Facilities and Biomass Conversion Processing for Fuels and Chemicals. Energy Conversion and Management, 41, 1357 1378
  35. 35. Drzymala Z. 1993Industrial briquetting- fundamentals and methods. Studies in mechanical engineering, 13Warszawa: PWN-Polish Scientific Publishers.
  36. 36. Encyclopædia Britannica. (2008). Cellulose. Retrieved May 23, 2008, from Encyclopædia Britannica Online.
  37. 37. Esteghlalian A. Hashimoto A. G. Fenske J. J. Penner M. H. 1997Modeling and optimization of the dilute-sulfuric-acid pre-treatment of corn stover, poplar and switchgrass. Bioresource Technology, 59, 129 136
  38. 38. Fan L. T. Gharpuray M. M. Lee Y. H. 1987In Cellulose Hydrolysis Biotechnology Monographs, 57, 149 187New York, NY: Springer-Verlag.
  39. 39. Fang Q. Bolloni I. Haque E. Spillman C. K. 1997 Comparison of energy efficiency between a roller mill and a hammer mill Applied Engineering in Agriculture 631 635
  40. 40. Fasina O. O. Bransby D. Wood C. W. 2006Flow properties of biomass feedstock. ASABE Annual International Meeting, Portland, Oregon, Paper 066149July 9 12pages.
  41. 41. Focher B. Marzetti A. Marsano E. Conio G. Tealdi A. Cosani A. Terbojevich M. 1998Regenerated and Graft Copolymer Fibres from Steam-Exploded Wheat Straw: Characterization and Properties. Journal of Applied Polymer Science, 67, 961 974
  42. 42. Fox D. J. Gray P. P. Dunn N. W. Warwick L. M. 1989Comparison of alkali and steam (acid) pre-treatments of lignocellulosic materials to increase enzymic susceptibility: Evaluation under optimized pre-treatment conditions. Journal of Chemical Technology & Biotechnology, 44, 135 146
  43. 43. Galbe M. Zacchi G. 2002 A review of the production of ethanol from softwood. Applied Microbiology and Biotechnology 618 628
  44. 44. Garcia-Cubero M. T. Gonzalez-Benito G. Indacoechea I. Coca M. Bolado S. 2009Effect of ozonolysis pre-treatment on enzymatic digestibility of wheat and rye straw. Bioresource Technology, 100, 1608 1613
  45. 45. Garcia-Aparicio M. P. Ballesteros I. Gonzalez A. Oliva J. M. Ballesteros M. Negro M. J. 2006Effect of inhibitors released during steam-explosion pre-treatment of barley straw on enzymatic hydrolysis. Applied Biochemistry and Biotechnology, 129(1-3), 278 288
  46. 46. Gelbrich, J., Mai, C. & Militz, H.2009Evaluation of Bacterial Wood Degradation by Fourier-Transform-Infrared (FTIR) Measurements, The study has been done within the EU-project BACPOLES (EVK4-CT-2001-00043) at the University of Gottingen (2009), 6 pages4
  47. 47. Gould J. M. 1984 Alkaline peroxide delignification of agricultural residues to enhance enzymatic saccharification Biotechnology and Bioengineering 46 52
  48. 48. Granada E. López González. L. M. Míguez J. L. Moran J. 2002 Fuel lignocellulosic briquettes, die design and products study Renewable Energy 561 573
  49. 49. Grous, W.R., Converse, A.O., & Grethlein, H.E.1985Effect of Stem Explosion Pre-treatment on Pore Size and Enzymatic Hydrolysis or Poplar. Enzyme Microbial Technology, 1986(8), 274 280
  50. 50. Harmsen, P.F.H., Huijgen, W.J.J., Bermudez Lopez, L.M., & Bakker, R.R.C.2010Literature Review of Physical and Chemical Pre-treatment Processes for Lignocellulosic Biomass. Energy Research Centre of the Netherlands. Report accessed on January 2010. Web Address: http://www.ecn.nl/docs/library/report/2010/e10013.pdf
  51. 51. Hatakka A. I. 1983Pre-treatment of wheat straw by white-rot fungi for enzymic saccharification of cellulose. Applied Microbiology and Biotechnology, 18, 350 357
  52. 52. Himmel M. Tucker M. Baker J. Rivard C. Oh K. Grohmann K. 1985Comminution of biomass: Hammer and knife mills. Biotechnology and Bioengineering Symposium, 15, 39 58
  53. 53. Hon D. N.S. 1989Cellulosic adhesives. In Adhesives from Renewable Resources, Eds. R.W. Hemmingway and A.H. Conner, 289 304Washington, DC: American Chemical Society.
  54. 54. Hu Z. Wen Z. 2008Enhancing enzymatic digestibility of switchgrass by microwave assisted alkali pre-treatment. Biochemical Engineering Journal, 38, 369 378
  55. 55. Hu Z. Wang Y. Wen Z. 2008Alkali (NaOH) Pre-treatment of switchgrass by radio frequency-based dielectric heating. Applied Biochemistry and Biotechnology, 148, 71 81
  56. 56. Igathinathane, C., Womac, A.R., Sokhansanj, S., & Narayan, S.2008 Bioresource Technology Knife grid size reduction to pre-process packed beds of high- and low-moisture switchgrass.,99,2254 2264
  57. 57. Jackson M. G. 1977The alkali treatment of straws. Animal Feed Science and Technology 105 130
  58. 58. Jin, S. & Chen, H.2006 Biochemical Engineering Journal Superfine Grinding of Steam-Exploded Rice Straw and its Enzymatic Hydrolysis.,30,225 230
  59. 59. Kaliyan N. Schmidt D. R. Morey R. V. 2010 Commercial Scale Grinding of Corn Stover and Perennial GrassesASABE Annual International Meeting, David L. Lawrence Convention Centre, Pittsburgh, Pennsylvania, June 20 23 Paper 1009062Niles Road, St. Joseph, MI 49085-9659 USA.
  60. 60. Kaliyan N. Morey R. V. 2006 Factors affecting strength and durability of densified products. ASABEAnnual International Meeting, American Society of Agricultural and Biological Engineers, Portland, Oregon July 9 12 Paper 066077Niles Road, St. Joseph, MI 49085-9659 USA.
  61. 61. Kashaninejad M. Tabil L. G. 2011 Effect of microwave-chemical pre-treatment on compression characteristics of biomass grinds Biosystems Engineering 36 45
  62. 62. Kelley, S.S., Rowell, R.M., Davis, M., Jurich, C.K., & Ibach, R.2004Rapid Analysis of the Chemical Composition of Agricultural Fibres Using Near Infrared Spectroscopy and Pyrolysis Molecular Beam Mass Spectrometry. Biomass and Bioenergy, 27(2004)77 88
  63. 63. Keshwani D. R. Cheng J. J. Burns J. C. Li L. Chiang V. 2007Microwave pre-treatment of switchgrass to enhance enzymatic hydrolysis. ASABE Annual Meeting Paper 077127Minneapolis, MN, USA.
  64. 64. Kitchaiya P. Intanakul P. Krairiksh M. 2003Enhancement of enzymatic hydrolysis of lignocellulosic wastes by microwave pre-treatment under atmospheric pressure. Journal of Wood Chemistry and Technology, 23(2), 217 225
  65. 65. Kokta B. V. Ahmed A. 1998Chapter 6: Steam Explosion Pulping. Environmentally Friendly Technologies for the Pulp and Paper Industry, edited by Raymond A. Young and Masood Akhtar, 0-47115-770-8Wiley and Sons, Inc.
  66. 66. Kumar P. Barrett D. M. Delwiche M. J. Stroeve P. 2009Methods for pre-treatment of lignocellulosic biomass for efficient hydrolysis and biofuel production. Industrial and Engineering Chemistry Research, 48, 3713 3729
  67. 67. Ladisch M. R. 1989Hydrolysis. In: Biomass Handbook. O. Kitani and C. W. Hall, eds. 434 451New York: Gordon and Breach.
  68. 68. Lam P. S. Sokhansanj S. Bi X. Lim C. J. Mani S. Melin S. 2008Energetic feasibility of biomass densification with steam explosion pretreatment. CSBE Annual General Meeting; July 14 16Poster CSBE08305Vancouver, BC.
  69. 69. Larkin S. Ramage J. Scurlock J. 2004Bioenergy. In: G. Boyle. ed. Renewable energy. Power for a sustainable future: 106 146p.
  70. 70. Larsson S. H. 2010 Kinematic Wall Friction Properties of Reed Canary Grass Powder at High and Low Normal Stresses Powder Technology 108 113
  71. 71. Larsson, S.H., Thyrel, M., Geladi, P., & Lestander, T.A.2008 Bioresource Technology High Quality Biofuel Pellet Production from Pre-Compacted Low Density Raw Materials.,99,7176 7182
  72. 72. Lebo, S. E. Jr., Gargulak, J.D., & McNally, T.J.2001“Lignin”. Kirk-Othmer Encyclopedia of Chemical Technology. John Wiley & Sons, Inc.DOI:10.1002/0471238961.12090714120914.a01.pub2Retrieved on 2007-10-14
  73. 73. Lehtikangas P. 2001Quality properties of palletized sawdust, logging residues and bark. Biomass and Bioenergy, 20, 351 360
  74. 74. Lesoing G. Klopfenstein T. Rush I. Ward J. 1980 Chemical treatment of wheat straw Journal of Animal Science, 51, 263 269
  75. 75. Lin Y. Tanaka S. 2006 Ethanol fermentation from biomass resources: current state and prospects Applied Microbiology and Biotechnology 627 642
  76. 76. Liu R. Yu H. Huang Y. 2005 Structure and Morphology of Cellulose in Wheat Straw Cellulose 25 34
  77. 77. Lopo P. 2002The right grinding solution for you: roll, horizontal or vertical. Feed Management, 53(3), 203 206
  78. 78. Luypaert, J., Zhang, M.H., & Massart, D.L.2003Feasibility Study for the Use of Near Infrared Spectroscopy in the Qualitative and Quantitative Analysis of Green Tea. Analytca Chimica Acta, 478(2003), 303 312
  79. 79. MacDonald, D.G., Bakhshi, N.N., Mathews, J.F., Roychowdhury, A., Bajpai, P., & Moo-Young, M.1983 Biotechnology and Bioengineering Alkali treatment of corn stover to improve sugar production by enzymatic hydrolysis,25,2067 2076
  80. 80. Magara K. Azuma J. 1989Microwave-irradiation of lignocellulosic materials X: Conversion of microwave-irradiated agricultural wastes into ethanol. Wood Research, 76, 1 9
  81. 81. Mani, S., Tabil, L.G., & Sokhansanj, S.2006 Biomass and Bioenergy, Effects of Compressive Force, Particle Size, and Moisture Content on Mechanical Properties of Biomass Pellets from Grasses.,30,648 654
  82. 82. Mani, S., Tabil, L.G., & Sokhansanj, S.2004 Biomass and Bioenergy Grinding performance and physical properties of wheat and barley straws, corn stover and switchgrass.,27,339 352
  83. 83. Mani S. Tabil L. G. Sokhansanj S. 2003An overview of compaction of biomass grinds. Powder Handling & Process, 15(3), 160 168
  84. 84. Marra F. Lyng J. Romano V. Mc Kenna B. 2007 Radio-frequency heating of foodstuff: Solution and validation of a mathematical model Journal of Food Engineering 998 1006
  85. 85. Mc Mullen J. Fasina O. O. Wood C. W. Feng Y. 2005 Storage and handling characteristics of pellets from poultry litter Applied Engineering in Agriculture 645 651
  86. 86. Mohsenin N. N. 1970 Physical Properties of Plant and Animal MaterialsNew York, N.Y.: Gordon and Breach Science Publishers.
  87. 87. Mosier N. Wyman C. Dale B. Elander R. Lee Y. Y. Holtzapple M. Ladisch M. 2005Features of promising technologies for pre-treatment of lignocellulosic biomass. Bioresource Technology, 96, 673 686
  88. 88. Murphy J. D. Mc Carthy K. 2005 Ethanol production from energy crops and wastes for use as a transport fuel in Ireland Applied Energy 148 166
  89. 89. Neely W. C. 1984Factors affecting the pre-treatment of biomass with gaseous ozone. Biotechnology and Bioengineering, 26, 59 65
  90. 90. Nelson D. L. Cox M. M. 2005 Lehninger Principles of BiochemistryNew York, NY: W.H. Freeman and Company.
  91. 91. Obernberger I. Thek G. 2004Physical characterization and chemical composition of densified biomass fuels with regard to their combustion behavior. Biomass and Bioenergy, 27, 653 669
  92. 92. Oberndorfer C. Pawelzik E. Lucke W. 2000 Prospects for the application of dielectric heating processes in the pre-treatment of oilseeds European Journal of Lipid Science and Technology 487 493
  93. 93. O’Dogherty M. J. 1982 A review of research on forage chopping Journal of Agricultural Engineering Research, 27(4), 267 289
  94. 94. Okano K. Kitagawa M. Sasaki Y. Watanabe T. 2005 Conversion of Japanese red cedar (Cryptomeria japonica) into a feed for ruminants by white-rot basidiomycetes Animal Feed Science and Technology 235 243
  95. 95. Ooshima H. Aso K. Harano Y. Yamamoto T. 1984 Microwave treatment of cellulosic materials for their enzymatic hydrolysis Biotechnology Letters 289 294
  96. 96. Overend R. P. Chornet E. 1987Fractionation of lignocellulosics by steam-aqueous pre-treatment. Philosophical Transactions of the Royal Society, London A 321, 523 536
  97. 97. Pfost H. B. Headley V. E. 1971Use of logarithmic normal distribution to describe hammer mill performance. Transactions of the ASABE, 14(3), 531 535
  98. 98. Puchalski C. Brusewitz G. H. 1996 Coefficient of friction of watermelon Transactions of the ASABE, 39(2), 589 594
  99. 99. Sánchez Ó. J. Cardona C. A. 2008 Trends in biotechnological production of fuel ethanol from different feedstocks Bioresource Technology 5270 5295
  100. 100. Schell D. J. Harwood C. 1994 Milling of Lignocellulosic Biomass: Results of Pilot-Scale Testing Applied Biochemistry and Biotechnology 159 168
  101. 101. Scholten R. L. Mc Ellhiney R. R. 1985The effects of prebreaking in hammer mill particle size reduction. American Society of Agricultural Engineers; Paper 85-3542 85 3542St. Joseph MI.
  102. 102. Seville J. P. K. Tuzun U. Clift R. 1997 Processing of Particulate SolidsLondon, U.K.: Chapman and Hall.
  103. 103. Shambe T. Kennedy J. F. 1985Acid and enzymatic hydrolysis of chaotropically pretreated millet stalk, acha and rice straws and conversion of the products to ethanol. Enzyme and Microbial Technology, 7, 115 120
  104. 104. Shaw M. 2008 Feedstock and Process Variables Influencing Biomass DensificationM.Sc. Thesis, Department of Agricultural and Bioresource Engineering, University of Saskatchewan. Website: http://library2.usask.ca/theses/available/etd-03092008115636 /unrestricted/Thesis.MarkShaw.FinalR3.pdf
  105. 105. Shaw M. D. Tabil L. G. 2006 Mechanical properties of selected biomass grindsASABE Annual International Meeting, Oregon Convention Center, Portland, Oregon, Paper 066175July 9-12: 12 pages.
  106. 106. Sherman Hsu. C. P. 1997Chapter 15: Infrared Spectroscopy, in: F. Settle, Editor, Handbook of Instrumental Techniques for Analytical Chemistry, Prentice-Hall, NJ 270.
  107. 107. Sitkei G. 1986 Mechanics of agricultural materialsAmsterdam: Elsevier.
  108. 108. Smola, N., & Urleb, U.2000 Analytica Chimica Acta Qualitative and Quantitative Analysis of Oxytetracycline by Near-Infrared Spectroscopy.410203 210
  109. 109. Sokhansanj S. Mani S. Bi X. Zaini P. Tabil L. G. 2005 Binderless pelletization of biomassASAE Annual International Meeting, Tampa Convention Centre, Tampa, Florida; July 17 20Paper 056061Niles Road, St. Joseph, MI 49085-9659 USA.
  110. 110. Soto M. L. Dominguez H. Nunez M. J. Lema J. M. 1994 Enzymatic saccharification of alkali-treated sunflower hulls Bioresource Technology 53 59
  111. 111. Soucek J. Hanzlikova I. Hulta P. 2003A fine disintegration of plants suitable for composite biofuels production. Research in Agricultural Engineering, 49(1), 7 11
  112. 112. Stenberg K. Tengborg C. Galbe M. Zacchi G. 1998Optimisation of steam pre-treatment of SO2-impregnated mixed softwoods for ethanol production. Journal of Chemical Technology and Biotechnology, 71(4), 299 308
  113. 113. Sun F. Chen H. 2007Evaluation of enzymatic hydrolysis of wheat straw pretreated by atmos-pheric glycerol autocatalysis. Journal of chemical technology and biotechnology, 82, 1039 1044
  114. 114. Sun Y. Cheng J. 2002 Hydrolysis of lignocellulosic materials for ethanol production: a review. Bioresource Technology 1 11
  115. 115. Tabil L. G. 1996Pelleting and binding characteristics of alfalfa. UnpublishedPh.D. thesis, Department of Agricultural and Bioresource Engineering, Saskatoon, SK Canada: University of Saskatchewan.
  116. 116. Taherzadeh M. J. Karimi K. 2007 Acid-based hydrolysis processes for ethanol from lignocellulosic materials: a review. Bioresources, 2, 472 499
  117. 117. Temmerman M. Rabier F. Jensen P. D. Hartmann H. Bohm T. 2006 Comparative Study of Durability Test Methods for Pellets and Briquettes Biomass and Bioenergy 964
  118. 118. Tomas-Pejo E. Oliva J. M. Ballesteros M. 2008 Realistic approach for full-scale bioethanol production from lignocellulose: a review Journal of Scientific & Industrial Research, 67, 874 884
  119. 119. Tripathi K. Iyer P. V. R. Kandpal T. C. 1988 A Techno-Economic Evaluation of Biomass Briquetting in India Biomass and Bioenergy 479 488
  120. 120. Tucker, M.P., Mitri, R.K., Eddy, F.P., Nguyen, Q.A., Gedvilas, L.M., & Webb, J.D.2000 Applied Biochemistry and Biotechnology Fourier Transform Infrared Quantification of Sugars in Pretreated Biomass Liquors.,84-86,39 50
  121. 121. United States Department of Energy (USDE).2006. Energy Efficiency and Renewable Energy- Biomass Program. Website Accessed on January 21, 2011. Web Address: http://www1.eere.energy.gov/biomass
  122. 122. Updegraff D. M. 1969 Semimicro Determination of Cellulose in Biological Materials. Analytical Biochemistry 420 424
  123. 123. van Dam J. E. G. van den Oever. M. J. A. Teunissen W. Keijsers E. R. P. Peralta A. G. 2004 Process for production of high density/high performance binderless boards from whole coconut huskPart 1: lignin as intrinsic thermosetting binder resin. Industrial Crops and Products 207 216
  124. 124. Vazquez, G., Gonzalez, J., Freire, S., & Antorrena, G.2002Characterization of Eucalyptus Globules and Pinus Pinaster Acetosolv Pulps Prebleached with O2 by FTIR and DRIFT Spectroscopy. Holz als Roh- und Werkstoff, 60(2002), 25 30
  125. 125. Vlasenko E. Y. Ding H. Labavitch J. M. Shoemaker S. P. 1997 Enzymatic Hydrolysis of Pretreated Rice Straw Bioresource Technology 109 119
  126. 126. Vidal P. F. Molinier J. 1988 Ozonolysis of lignin-improvement of in vitro digestibility of poplar sawdust. Biomass 1 17
  127. 127. Vigneault C. Rothwell T. M. Bourgeois G. 1992Hammer mill grinding rate and energy requirements for thin and conventional hammers. Canadian Biosystems Engineering, 34, 203 206
  128. 128. Viola, E., Zimbardi, F., Cardinale, M., Cardinale, G., Braccio, G., & Gambacorta, E.2008 Bioresource Technology Processing Cereal Straws by Steam Explosion in a Pilot Plant to Enhance Digestibility in Ruminants,99,681 689
  129. 129. Womac A. R. Igathinathane C. Bitra P. Miu P. Yang T. Sokhansanj S. Narayan S. 2007 Biomass Pre-Processing Size Reduction with Instrumented MillsASABE Annual International Meeting, Minneapolis Convention Centre, Minneapolis, June 17 20Paper 076046Niles Road, St. Joseph, MI 49085-9659 USA.
  130. 130. Zandersons J. Gravitis J. Zhurinsh A. Kokorevics A. Kallavus U. Suzuki C. K. 2004 Carbon materials obtained from self-binding sugar cane bagasse and deciduous wood residues plastics Biomass and Bioenergy 345 360
  131. 131. Zimbardi F. Viola E. Nanna F. Larocca E. Cardinale M. Barisano D. 2007 Acid impregnation and steam explosion of corn stover in batch processes Industrial Crops and Products 195 206
  132. 132. Zimbardi F. Viggiano D. Nanna F. Demichele M. Cuna D. Cardinale G. 1999 Steam Explosion of Straw in Batch and Continuous Systems Applied Biochemistry and Biotechnology 117 125
  133. 133. Zhu, S., Wu, Y., Yu, Z., Zhang, X., Li, H., & Gao, M.2006a Bioresource Technology, The effect of microwave irradiation on enzymatic hydrolysis of rice straw.,97,1964 1968
  134. 134. Zhu S. Wu Y. Yu Z. Chen Q. Wu G. Yu F. Wang C. Jin S. 2006b Microwave-assisted alkali pre-treatment of wheat straw and its enzymatic hydrolysis Biosystems Engineering 437 442
  135. 135. Zhu S. Wu Y. Yu Z. Zhang X. Wang C. Yu F. Jin S. 2006c Production of ethanol from microwave-assisted alkali pretreated wheat straw Process Biochemistry 869 873
  136. 136. Zhu S. Wu Y. Yu Z. Liao J. Zhang Y. 2005Pre-treatment by microwave/alkali of rice straw and its enzymic hydrolysis. Process Biochemistry, 40, 3082 3086

Written By

Lope Tabil, Phani Adapa and Mahdi Kashaninejad

Submitted: 18 October 2010 Published: 01 August 2011